HASTELLOY® X /GH3536(UNS N06002/W-Nr 2.4665 )
HASTELLOY® X /GH3536(UNS N06002/W-Nr 2.4665 )特性:
合金在1200℃的高温下,仍具有极高的强度和耐氧化性,加上出色的成型及焊接性能,和出色的耐应力腐蚀开裂性能,被广泛用于燃气轮机,工业炉,热处理设备和核工程的过程组件,如燃气涡轮的燃烧缸、补燃器锥管、过渡管、喷射杆,以及化工行业的蒸馏,马弗炉,催化剂支撑格栅,炉膛挡板,热解操作的管材和闪蒸干燥器部件等。
HASTELLOY® X /GH3536(UNS N06002/W-Nr 2.4665 )牌号标准名称:
| 中国 | GB/T 14992-2005 | GH3536(GH536) | 
| 美国 | ASTM B572-2011 | UNS N06002 | 
| HAYNES | HASTELLOY® X alloy | |
| 日本 | JIS H 4551-2000 | NW6002 NiCr21Fe18Mo9 | 
| NIPPON YAKIN | NAS HX | |
| 德国 | DIN 17744-2002 | 2.4665 NiCr22Fe18Mo | 
| VDM Metals | Nicrofer®4722 Co alloy X | 
| 牌号 | GH3536 | N06002 | NW6002 | 2.4665 | 
| C | 0.05~0.15 | 0.05~0.15 | 0.05~0.15 | 0.05~0.15 | 
| Si | ≤1.00 | ≤1.00 | ≤1.00 | ≤1.00 | 
| Mn | ≤1.00 | ≤1.00 | ≤1.00 | ≤1.00 | 
| P | ≤0.025 | ≤0.040 | ≤0.040 | ≤0.020 | 
| S | ≤0.015 | ≤0.030 | ≤0.015 | |
| Ni | 余量 | Remainder | 残部 | Other | 
| Cr | 20.5~23.0 | 20.5~23.0 | 20.5~23.0 | 20.5~23.0 | 
| Mo | 8.0~10.0 | 8.0~10.0 | 8.0~10.0 | 8.0~10.0 | 
| Fe | 17.0~20.0 | 17.0~20.0 | 17.0~20.0 | 17.0~20.0 | 
| Co | 0.5~2.5 | 0.5~2.5 | 0.5~2.5 | 0.5~2.5 | 
| W | 0.2~1.0 | 0.2~1.0 | 0.2~1.0 | 0.2~1.0 | 
| Al | ≤0.50 | — | — | ≤0.50 | 
| Ti | ≤0.15 | — | — | — | 
| Cu | ≤0.50 | — | — | ≤0.50 | 
| B | ≤0.01 | — | ≤0.01 | ≤0.01 | 
化学成分:
| 牌号 | GH3536 | N06002 | NW6002 | 2.4665 | 
| C | 0.05~0.15 | 0.05~0.15 | 0.05~0.15 | 0.05~0.15 | 
| Si | ≤1.00 | ≤1.00 | ≤1.00 | ≤1.00 | 
| Mn | ≤1.00 | ≤1.00 | ≤1.00 | ≤1.00 | 
| P | ≤0.025 | ≤0.040 | ≤0.040 | ≤0.020 | 
| S | ≤0.015 | ≤0.030 | ≤0.015 | |
| Ni | 余量 | Remainder | 残部 | Other | 
| Cr | 20.5~23.0 | 20.5~23.0 | 20.5~23.0 | 20.5~23.0 | 
| Mo | 8.0~10.0 | 8.0~10.0 | 8.0~10.0 | 8.0~10.0 | 
| Fe | 17.0~20.0 | 17.0~20.0 | 17.0~20.0 | 17.0~20.0 | 
| Co | 0.5~2.5 | 0.5~2.5 | 0.5~2.5 | 0.5~2.5 | 
| W | 0.2~1.0 | 0.2~1.0 | 0.2~1.0 | 0.2~1.0 | 
| Al | ≤0.50 | — | — | ≤0.50 | 
| Ti | ≤0.15 | — | — | — | 
| Cu | ≤0.50 | — | — | ≤0.50 | 
| B | ≤0.01 | — | ≤0.01 | ≤0.01 | 
| 牌号 | GH3536 | N06002 | NW6002 | 2.4665 | 
| C | 0.05~0.15 | 0.05~0.15 | 0.05~0.15 | 0.05~0.15 | 
| Si | ≤1.00 | ≤1.00 | ≤1.00 | ≤1.00 | 
| Mn | ≤1.00 | ≤1.00 | ≤1.00 | ≤1.00 | 
| P | ≤0.025 | ≤0.040 | ≤0.040 | ≤0.020 | 
| S | ≤0.015 | ≤0.030 | ≤0.015 | |
| Ni | 余量 | Remainder | 残部 | Other | 
| Cr | 20.5~23.0 | 20.5~23.0 | 20.5~23.0 | 20.5~23.0 | 
| Mo | 8.0~10.0 | 8.0~10.0 | 8.0~10.0 | 8.0~10.0 | 
| Fe | 17.0~20.0 | 17.0~20.0 | 17.0~20.0 | 17.0~20.0 | 
| Co | 0.5~2.5 | 0.5~2.5 | 0.5~2.5 | 0.5~2.5 | 
| W | 0.2~1.0 | 0.2~1.0 | 0.2~1.0 | 0.2~1.0 | 
| Al | ≤0.50 | — | — | ≤0.50 | 
| Ti | ≤0.15 | — | — | — | 
| Cu | ≤0.50 | — | — | ≤0.50 | 
| B | ≤0.01 | — | ≤0.01 | ≤0.01 | 
HASTELLOY® X /GH3536(UNS N06002/W-Nr 2.4665 )应用:
是主要用铬和钼固溶强化的一种铁量较高的镍基高温合金,密度为8.3g/cm3。